Technical Reference Library

Ni-Hard Cast Iron

ASTM A532 Class IType Ni-Cr white cast ironHardness 500 HB and up

In short: Ni-Hard is a family of nickel-chromium martensitic white cast irons built for abrasion in crushing and grinding equipment, grinding balls included. ASTM A532 Class I covers them, and Type A is the classic Ni-Hard 1. Hardness starts around 500 HB sand cast and reaches 600 HB and more chill cast, which puts hardened Ni-Hard beyond standard carbide. It is ground, or machined with PCBN.

Material Overview

The nickel-chromium white irons, sold as Ni-Hard, are the oldest group of high-alloy irons of industrial importance and have been made for more than 50 years. Nickel is the main alloying element and produces a martensitic matrix around hard carbides. They are commonly identified as Ni-Hard types 1 to 4 and are used for crushing and grinding.

ASTM A532 covers white cast irons alloyed for abrasion resistance in mining, milling, earth-handling and manufacturing. Castings can be supplied as cast, as cast and stress relieved, hardened, hardened and stress relieved, or softened for machining.

Chemical Composition: ASTM A532 Class I Type A (Ni-Hard 1)

Element Content
Carbon (C) 2.8 to 3.6%
Manganese (Mn) 2.0% max
Silicon (Si) 0.8% max
Nickel (Ni) 3.3 to 5.0%
Chromium (Cr) 1.4 to 4.0%
Molybdenum (Mo) 1.0% max

Source: ASTM A532/A532M Table 1, Class I Type A (Ni-Cr-Hc).

Ni-Hard hardness

Condition Hardness
Ni-Hard, sand cast and stress relieved 500 HB minimum
Ni-Hard, chill cast and stress relieved 600 HB minimum
High-alloy white irons in general 450 to 800 HB

Sources: US Patent 4,338,128 (Ni-Hard description); white iron overview citing ASTM A532. See our hardness conversion chart for HRC equivalents.

Machining Ni-Hard

Hardened Ni-Hard is not a job for standard carbide inserts. The two practical routes are grinding and PCBN. Polycrystalline cubic boron nitride is widely used for machining hard, abrasive white irons, and thicker solid PCBN inserts now rough white iron that used to be ground only, with depths of cut up to about 3/16 in. and a heavy T-land edge prep (around 0.150 in. x 15°) for roughing.

If a part needs heavy machining, ask the foundry about supplying it in the softened-for-machining condition and hardening it afterward, which A532 allows.

Ni-Hard Cast Iron questions

What is Ni-Hard?

Ni-Hard is the trade name for a family of nickel-chromium martensitic white cast irons used where abrasion is the main problem, such as crushing and grinding equipment. ASTM A532 Class I covers it; Type A is Ni-Hard 1.

How hard is Ni-Hard?

Ni-Hard has a minimum of about 500 HB sand cast and stress relieved, and 600 HB chill cast and stress relieved. High-alloy white irons in general range from 450 to 800 HB.

Can Ni-Hard be machined?

Not with standard carbide once hardened. It is ground or machined with PCBN inserts, which can rough white iron at depths of cut up to about 3/16 in. A532 also allows castings to be supplied softened for machining and hardened afterward.

What is the composition of Ni-Hard 1?

ASTM A532 Class I Type A: 2.8 to 3.6% carbon, 3.3 to 5.0% nickel, 1.4 to 4.0% chromium, 2.0% max manganese, 0.8% max silicon and 1.0% max molybdenum.

Get tooling tips by email

New TechTips, TechTalks and tool releases. No spam.