ASTM A216 WCB Cast Steel
In short: ASTM A216 WCB is the most widely used cast carbon steel for pressure-containing parts: valve bodies, pump casings, fittings. The spec limits carbon to 0.30% and requires 70 to 95 ksi tensile strength with 36 ksi minimum yield, and every casting must be heat treated (annealed, normalized, or normalized and tempered). In the shop it machines like a low-carbon steel once you are under the cast skin, so the real work is getting through that first pass cleanly.
Material Overview
ASTM A216 covers carbon steel castings for valves, flanges, fittings and other pressure-containing parts in high-temperature service. It has three grades: WCA, WCB and WCC. WCB is the one most valve specifications call for, including gate, globe and check valve bodies built to API 600, API 602 and BS 1868, and ball valve bodies to API 6D and API 608.
Castings are furnished annealed, normalized, or normalized and tempered, and heat treatment is done after the casting has cooled below the transformation range. The commonly quoted service range is -20 °F to 800 °F (-29 °C to 425 °C).
Chemical Composition (Grade WCB)
| Element | Content |
|---|---|
| Carbon (C) | 0.30% max |
| Manganese (Mn) | 1.00% max |
| Silicon (Si) | 0.60% max |
| Phosphorus (P) | 0.035% max |
| Sulfur (S) | 0.035% max |
| Residuals: Cu / Ni / Cr | 0.30 / 0.50 / 0.50% max |
| Residuals: Mo / V | 0.20 / 0.03% max |
| Total residual elements | 1.00% max |
Source: ASTM A216/A216M Table 1.
Mechanical Properties: WCA vs WCB vs WCC
| Property | WCA | WCB | WCC |
|---|---|---|---|
| Tensile strength | 60 to 85 ksi (415 to 585 MPa) | 70 to 95 ksi (485 to 655 MPa) | 70 to 95 ksi (485 to 655 MPa) |
| Yield strength (min) | 30 ksi (205 MPa) | 36 ksi (250 MPa) | 40 ksi (275 MPa) |
| Elongation in 2 in. (min) | 24% | 22% | 22% |
| Reduction of area (min) | 35% | 35% | 35% |
| UNS | J02502 | J03002 | J02503 |
Source: ASTM A216/A216M Table 2. Always check the mill certificate for your heat.
Machining A216 WCB
Under the skin, WCB is a low-carbon steel (ISO P group) and cuts much like Steel 1020, so that page is a sensible starting point for speeds. The difference is the outside of the casting: scale, burned-in sand and hard spots from the mold. Set the first depth of cut deep enough to get under the skin in one pass instead of rubbing on it, choose a tough grade and a strong edge for that pass, and save the sharper, harder grade for finishing.
Valve bodies are often interrupted cuts (ports, flanges, bolt bosses), and a rigid setup matters more than speed. If chips are long and stringy on finishing passes, a chipbreaker designed for low-carbon steel will help.
ASTM A216 WCB Cast Steel questions
What is ASTM A216 WCB?
It is a cast carbon steel grade defined by ASTM A216 for pressure-containing parts such as valve bodies, flanges and fittings in high-temperature service. It is the most common cast steel in valve specifications.
What is the difference between WCB and WCC?
WCC has a higher minimum yield strength (40 ksi vs 36 ksi) and a lower carbon limit (0.25% vs 0.30%) with more manganese allowed (1.20% vs 1.00%). Tensile strength range is the same, 70 to 95 ksi.
What is the UNS number for WCB?
ASTM A216 Grade WCB is UNS J03002. WCA is J02502 and WCC is J02503.
What temperature range is A216 WCB used for?
WCB is commonly specified from -20 °F to 800 °F (-29 °C to 425 °C).
How do you machine A216 WCB?
Treat it as a low-carbon steel with a cast skin. Take the first cut deep enough to get under the scale and sand in one pass, use a tough carbide grade for that pass, and finish with a sharper edge. Our Steel 1020 page gives starting cutting speeds.