ASTM A36 Steel
In short: ASTM A36 is the standard carbon structural steel in the United States, used for plate, bars and shapes in general construction and fabrication. It is specified mainly by strength: 36 ksi minimum yield and 58 to 80 ksi tensile. Chemistry limits are maximums that change with thickness (carbon 0.25% to 0.29% for plate). In the shop it behaves like a mild, low-carbon steel.
Material Overview
A36 is the Standard Specification for Carbon Structural Steel, used for shapes, plates and bars in general construction and structural applications. Because the spec is written around tensile requirements, two heats of A36 can differ in chemistry while both comply. Welders and fabricators often group it with SAE 1020 as plain carbon steel.
Plates, bars and shapes up to 8 in. thick must reach 36 ksi minimum yield; plates thicker than 8 in. drop to 32 ksi with the same 58 to 80 ksi tensile range.
Chemical Composition (plates)
| Element | Up to 3/4 in. | 3/4 to 1-1/2 in. | 1-1/2 to 2-1/2 in. | 2-1/2 to 4 in. | Over 4 in. |
|---|---|---|---|---|---|
| Carbon (max) | 0.25% | 0.25% | 0.26% | 0.27% | 0.29% |
| Silicon | 0.40% max | 0.40% max | 0.15 to 0.40% | 0.15 to 0.40% | 0.15 to 0.40% |
| Phosphorus (max) | 0.04% | 0.04% | 0.04% | 0.04% | 0.04% |
| Sulfur (max) | 0.05% | 0.05% | 0.05% | 0.05% | 0.05% |
| Copper (when copper steel is specified) | 0.20% min | 0.20% min | 0.20% min | 0.20% min | 0.20% min |
Source: ASTM A36/A36M chemical requirements for plates. Shapes allow 0.26% carbon max.
ASTM A36 mechanical properties
| Property | Value |
|---|---|
| Tensile strength | 58 to 80 ksi (400 to 550 MPa) |
| Yield point (min) | 36 ksi (250 MPa); 32 ksi (220 MPa) for plates over 8 in. |
| Elongation, plates and bars (min) | 23% in 2 in.; 20% in 8 in. |
| Modulus of elasticity | 29,000 ksi (200 GPa) |
| Shear modulus | 11,300 ksi (78 GPa) |
| Poisson's ratio | 0.32 |
Source: ASTM A36/A36M tensile requirements. Always check the mill certificate for your heat.
Machining A36
A36 is a low-carbon steel (ISO P group) and machines much like Steel 1020, which is the best starting point for cutting speeds. Hot-rolled plate and bar carry mill scale; take the first pass under it rather than skimming it. The soft, ductile matrix tends to form long chips and built-up edge at low speed, so run carbide at a proper surface speed and use a chipbreaker designed for mild steel.
ASTM A36 Steel questions
What is the yield strength of A36 steel?
36 ksi (250 MPa) minimum for plates, bars and shapes up to 8 in. thick. Plates over 8 in. have a 32 ksi (220 MPa) minimum. Tensile strength is 58 to 80 ksi (400 to 550 MPa) in both cases.
Is A36 the same as 1018 or 1020?
No. A36 is a structural specification defined mainly by strength, with only maximum limits on chemistry. SAE 1018 and 1020 are defined by chemical composition. They are all low-carbon steels and machine in a similar way, but they are not interchangeable on a drawing.
What is the UNS number for A36?
ASTM A36 steel is UNS K02600.
How do you machine A36 steel?
Treat it as a mild, low-carbon steel. Cut under the mill scale on the first pass, keep surface speed high enough to avoid built-up edge, and use a chipbreaker for mild steel. Our Steel 1020 page lists starting cutting speeds.